One cannot simply judge that the 800/900 series of product condensation mold silicone rubber (100:2 two-component liquid silicone rubber with high tear strength or capable of being molded multiple times) is suitable for all plaster, cement, POLY-RESIN, PU, AB water, ABS material mold systems based solely on its being 100:2 in weight ratio, high tear strength, or the ability to be molded multiple times. One must first confirm the A/B weight ratio, the state of the curing agent and the uniformity of the mixing, the material of the mother mold and the mold frame, the compatibility of the release agent, vacuum degassing, the method of releasing the glue, the curing temperature and time, and the hardness requirements of the product. Then, one can determine whether the problem lies in the deviation of the ratio, the evaporation of the curing agent, improper treatment of the mother mold, the residual bubbles, or the mismatch in the compatibility with the resin and the mold conditions. The 800/900 series of product mold silicone rubber can be considered as a candidate for condensation mold silicone rubber, but it must be confirmed through small-scale tests, degassing verification, and actual mold molding tests.
Why do condensation mold silicone rubber often have fewer moldings or fail to cure during moldings?
If A/B is not accurately weighed in a 100:2 ratio or approximated by volume ratio, it leads to incomplete curing, low hardness, or sticky surfaces.
If the curing agent is not thoroughly mixed, there is an excess or insufficient amount of curing agent in some areas, resulting in uneven curing, sticky areas, or brittleness.
If the glue is heated immediately after pouring, the curing agent evaporates prematurely, causing the glue to fail to cure or cure incompletely.
If the surface of the mother mold or mold frame is not cleaned, there are oil stains, dust, or residual release agents, which affect the wetting of the glue and the release process, making it prone to tearing during moldings.
If the degassing process is not carried out, there are residual bubbles in the details of the mother mold, and during moldings, the bubble areas become stress concentration points, causing the mold to be prone to damage.
If the pouring method is improper, such as pouring all at once or from a low position, the glue has insufficient flow time and is severely adhered.
If the material of the mold frame is not smooth or has poor compatibility with the silicone rubber, the mold will be pulled apart during the molding process, reducing the number of moldings.
If the mold is removed after less than 8-10 hours of curing, the glue layer has not fully cross-linked, and the tear resistance has not been fully exerted.
When switching from add-on mold glue, 10:1 mold glue, or other condensation mold silicone rubber to another type, if the ratio, degassing, and curing conditions are not re-adjusted, the mold molding performance may deviate from the target.
Contacting compounds such as tin, phosphorus, ammonium, chlorine, carboxylic acid, thiol, hydroxyl, etc., or if the curing agent is damp or expired, it affects the curing quality.
If the storage conditions are improper or exceed the shelf life, the activity of the A/B components decreases, affecting the consistency of curing and the lifespan of moldings.
If there are clear requirements for moldings or tear resistance or solvent resistance, but the actual resin type and mold conditions are not verified.
First, determine at which stage the moldings or low curing occurs.
Failure stage Possible causes Priority inspection direction
Glue does not cure or is not fully cured after mixing A/B ratio deviation, uncured curing agent, curing agent evaporation or expiration Accuracy of ratio, mixing method, curing agent state
Glue fails to cure immediately after pouring Early curing agent evaporation Heating timing, curing temperature curve
There are bubbles or spots on the mold surface No vacuum degassing, improper pouring method, unclean mother mold Degassing process, pouring height, mold treatment
There are bubbles or insufficient glue in the details of the mold Insufficient glue flow time, high viscosity, complex mold structure Pouring method, glue viscosity, mold exhaust
The mold tears or moldings occur with few times Insufficient tear resistance, insufficient curing, improper release agent, rough mold frame Model selection, curing time, release agent, mold frame material
Mold shrinkage or size deviation Excessive curing temperature, thick glue layer, unverified shrinkage rate Verification of curing temperature, glue layer thickness, size
The mold is swollen or corroded after contacting the resin Insufficient solvent resistance, excessive resin heat release, incompatible release agent Resin type, solvent verification, release agent
Batch-to-batch curing or fluctuation in moldings lifespan A/B component activity difference, storage conditions, measurement error Inspection during entry, storage records, measurement accuracy
If only the "whether the product mold silicone 800/900 series was used" is considered without recording the A/B weight ratio, the curing agent status, bubble removal, pouring method, curing time, and mold handling, it is usually difficult to accurately determine whether it is a material issue or a process issue.
Why is increasing the curing agent dosage or raising the curing temperature not necessarily effective?
The product mold silicone 800/900 series plays a condensation curing role in the mold flipping system. It is affected by the ratio, the curing agent status, bubble removal, pouring method, and curing conditions. Simply increasing the curing agent dosage or raising the temperature may bring side effects.
Increasing the curing agent dosage may accelerate the curing process, but excessive dosage will cause the mold to be too brittle, the anti-tear strength to decrease, and the mold flipping frequency to decrease instead.
Reducing the curing agent dosage may lead to incomplete curing, a sticky surface, and insufficient mold strength.
Heating immediately after pouring will accelerate the evaporation of the curing agent, resulting in incomplete curing or inability to cure.
Increasing the curing temperature may shorten the curing time, but it may cause an increase in mold shrinkage, deformation of the mother mold, or a decrease in solvent resistance.
Increasing the total dosage of A/B does not change the 100:2 weight ratio requirement. Excessive resin will not increase the mold flipping life but will cause waste.
When not vacuuming to remove bubbles, adjusting only the curing agent or temperature cannot eliminate the blistering at the mold details.
If the mold surface is not cleaned or the release agent is inappropriate, adjusting only the curing conditions cannot solve the problem of mold tearing.
After storage has expired or the curing agent has been damp, adjusting the ratio alone cannot restore the original curing performance.
Therefore, when optimizing, one should observe the A/B weight ratio, the curing agent status, the mixing method, vacuum bubble removal, pouring method, mold handling, curing temperature and time, rather than only adjusting a single parameter.
How should different models of product mold silicone 800/900 be selected?
Working conditions Product mold silicone 800/900 candidate direction Product mold silicone 805/905 candidate direction Product mold silicone 810/910 candidate direction Product mold silicone 815/915 candidate direction Product mold silicone 820/920 candidate direction Product mold silicone 825/925 candidate direction Product mold silicone 830/930 candidate direction Still need verification
Ultra-soft high-elastic simulation molds Hardness 0±2, elongation 580±50%, suitable for soft simulation Hardness 5±2, elongation 550±50% Hardness 10±2, elongation 500±50% Hardness 15±2, elongation 450±50% Hardness 20±2, elongation 420±50% Hardness 25±2, elongation 400±50% Hardness 30-35, elongation 300±50% Release performance, detail replication, anti-tear
High anti-tear and wear-resistant molds Anti-tear 5±2 kN/m Anti-tear 8±2 kN/m Anti-tear 10±2 kN/m Anti-tear 15±2 kN/m Anti-tear 20±2 kN/m Anti-tear 23±2 kN/m Anti-tear 22±2 kN/m Actual anti-tear, fatigue resistance, mold flipping frequency
Low viscosity easy bubble removal Viscosity 8000-10000 cps Viscosity 8000-10000 cps Viscosity 8000-10000 cps Viscosity 15000±2000 cps Viscosity 20000±2000 cps Viscosity 23000±2000 cps Viscosity 25000±2000 cps Vacuum degree, bubble removal time, bubble residue
High tensile strength requirements Tensile 2.03 MPa Tensile 2.12 MPa Tensile 2.46 MPa Tensile 2.56 MPa Tensile 2.57 MPa Tensile 3.98 MPa, maximum tensile Tensile 3.17 MPa Actual tensile, elongation at break, modulus
Gypsum, cement, POLY-RESIN, PU, AB water, ABS - Need to verify chemical resistance and demolding properties - Need to verify - Need to verify - Need to verify - Need to verify - Need to verify - Resin type, heat release temperature, demolding agent
Oil sludge, toys, gifts, relief sculptures, Buddha statues, sculptures - Soft and highly elastic, suitable for detailed demolding - General fine replication - General fine replication - Higher hardness, stable size - Higher hardness, suitable for large items - Higher hardness, high tear resistance - Higher hardness, high support - Mother mold details, shrinkage rate, mold flipping life
Do not just choose based on hardness, as the viscosity, tear resistance, tensile and elongation rates of the 7 models vary. The final choice depends on the mother mold structure, resin type, demolding difficulty, mold flipping times and bubble removal process.
What are the differences in product mold silicone 800/900 series selection compared to injection molding mold glue and similar condensation-type mold glue?
Comparison direction Product mold silicone 800/900 series (100:2 condensation type) Highly transparent injection molding glue (10:1) High-temperature resistant injection molding glue (1:1) General condensation-type mold glue Selection boundary
Ratio 100:2 weight ratio 10:1 weight ratio 1:1 weight ratio Depending on the product Ratio different, need to re-adjust measurement and mixing process when switching
Curing mechanism Condensation type, curing agent cross-linking Platinum injection molding Platinum injection molding Condensation type Condensation type sensitive to curing agent and moisture, injection molding sensitive to platinum toxic substances
High-temperature resistance Resistant to burning, high-temperature, corrosion, solvents Unmarked high-temperature resistant baking molds Resistant to 250°C, 200°C for long-term stability General High-temperature injection molding glue preferred for baking molds
Transparency White/semi-transparent High transparency Translucent General High transparency injection molding glue preferred for high transparency products
Shrinkage rate ≤0.3% Almost no shrinkage ≤0.1% Shrinkage is large High dimensional stability requires priority for injection molding
Mold flipping times Information mentions multiple mold flipping times Need to verify Need to verify General Need to verify based on actual resin and demolding method
Bubble removal requirements Need to vacuum for bubble removal High viscosity models need to strengthen vacuum bubble removal Over 20 hardness recommends vacuum removal Lower viscosity is easy to remove bubbles Choose according to vacuum equipment and mold structure
Curing agent/catalyst sensitivity Sensitive to curing agent ratio, volatility, moisture absorption Sensitive to tin, phosphorus, ammonium, chlorine, etc. platinum toxic substances Sensitive to tin, phosphorus, ammonium, chlorine, etc. platinum toxic substances Sensitive to curing agent Strictly manage ratio and pollution sources according to the system
Operation time 15-25 minutes 60±10 minutes 30-40 minutes Depending on the product Choose based on the pouring and bubble removal rhythm
Applicable scenarios Gypsum, cement, POLY-RESIN, PU, AB water, ABS molds High-precision molds, resin ornaments, fine product replication High-temperature baking molds, high-temperature simulation General molds Choose based on resin type, high-temperature resistance and transparency
Why is it still necessary to conduct complete tests when compatibility with the mother mold and curing agent is ensured?
Our company's public information states that the product mold silicone 800/900 series is used as elastic mold materials for pouring gypsum, cement, POLY-RESIN, PU, AB water, ABS materials, as well as for the production and replication of oil sludge, toys, gifts, relief sculptures, Buddha statues, urban sculptures, cement products, hand boards, car models, household appliance models, soap molds, etc. However, when used in actual systems, there may still be:
Mother mold material, surface treatment and demolding agent differences.
Frame material, smoothness and sealing material.
A/B weight ratio, curing agent type and state.
Mixing method, vacuum bubble removal and pouring method.
Curing temperature, time and layer thickness of the glue.
Resin type, heat release temperature and demolding agent compatibility.
Mold flipping times, demolding method and mold life.
Environmental cleanliness, dust and fiber contamination.
Storage conditions and the activity of A/B components.
Batch-to-batch consistency of curing and mold flipping performance.
Uniform appearance or short-term curing compliance, but cannot prove long-term mold flipping, resistance to resin heat release or stability after repeated demolding. Before use, verification should be conducted using a complete formulation, actual mother mold and resin conditions.
Which parameters should be confirmed when using the product mold silicone 800/900 series?
Parameter category Required information
Application direction Gypsum, cement, POLY-RESIN, PU, AB water, ABS molds, oil clay, toys, gifts, relief, Buddha statues, sculptures, etc.
Mother mold type Oil clay, resin, gypsum, wood, 3D printed parts, etc.
Surface treatment Cleaning method, type of release agent, presence of oil and dust
Frame material Acrylic board and other smooth materials, compatibility of sealing materials with silicone
A/B ratio 100:2 weight ratio, measurement accuracy and mixing uniformity
Curing agent status Type, whether damp, whether expired, uniformity of stirring
Stirring method Same direction stirring, stirring time, avoiding air entrapment
Vacuum degassing Vacuum degree, degassing time, viscosity and temperature of the adhesive
Pouring adhesive method Adhesive pouring height, pouring position, natural leveling
Curing conditions 8-10 hours at room temperature or 6-8 hours, whether heating and heating timing
Model selection 800/900 - 830/930 and target hardness, tensile strength, viscosity, elongation
Resin type Gypsum, cement, POLY-RESIN, PU, AB water, ABS
Storage conditions Cold and dry, sealed, use according to expiration date
Acceptance indicators Bubbles, hardness, tensile strength, elongation, shrinkage rate, demolding performance, mold flipping times
What should be focused on verifying when using the product mold silicone 800/900 series?
A/B weight ratio measurement accuracy and curing agent stirring uniformity.
Content of bubbles in the cured adhesive after stirring and vacuum degassing effect.
Coating of bubbles on the details of the mother mold and surface blemishes after pouring adhesive.
Hardness, tensile strength and elongation after curing.
Actual performance of elongation and shrinkage rate ≤ 0.3%.
Demolding and dimensional stability of the mold and mother mold.
Chemical resistance and demolding performance after pouring gypsum, cement, POLY-RESIN, PU, AB water, ABS.
Mold flipping times and mold tearing and wear conditions.
Impact of mold curing agent getting damp, expiring or immediate heating after pouring adhesive.
Matching of viscosity with degassing and pouring adhesive process for different hardness models.
Batch-to-batch consistency of curing and mold flipping performance fluctuations.
Curing speed of A/B components after storage.
How to design experiments before using the product mold silicone 800/900 series?
Establish a current mold silicone benchmark, record model, A/B ratio, curing agent status, degassing, pouring adhesive and curing conditions and failure manifestations.
Uniform test conditions: mother mold, surface treatment, frame material, A/B ratio, stirring method, vacuum degassing, pouring adhesive method, curing temperature and time.
Set candidate samples: current mold adhesive, product mold silicone 800/900 series of different hardness models, different degassing and curing conditions gradients.
Complete the entire process test: mixing - vacuum degassing - pouring adhesive - curing - demolding - bubble/mechanical property testing - mold flipping verification.
Evaluate actual results: bubbles, hardness, tensile strength, elongation, shrinkage rate, demolding performance, mold flipping times.
Test items Uniform requirements
Mother mold and surface treatment Consistent
Frame material Consistent or set according to test design
A/B ratio 100:2 weight ratio
Curing agent status Consistent, record damp and expired situations
Stirring and degassing process Set gradient according to test design
Pouring adhesive method Set gradient according to test design
Curing conditions: Set the gradient according to the test design, avoiding heating immediately after gelation.
Measurement methods: Bubble, hardness, tear resistance, tensile strength, elongation rate, shrinkage rate, demolding property, number of demolding cycles are consistent.
Which situations are not suitable for directly using the product mold silicone 800/900 series?
A/B weight ratio measurement accuracy cannot be guaranteed or approximate proportion is made based on volume ratio, resulting in incomplete curing.
Curing agent gets damp, expires, or is not stirred evenly, leading to poor curing or local stickiness.
Heating immediately after gelation accelerates curing, causing the curing agent to volatilize and unable to cure.
No vacuum degassing was performed, and bubbles remain in the details of the mother mold, making it prone to tearing during demolding.
Common Misconceptions
100:2 can be approximately proportioned by volume ratio
The product proportion is 100:2 by weight ratio. Proportioning by volume ratio approximately may lead to deviation in proportion, affecting the complete curing and the lifespan of the mold. It is necessary to accurately weigh by weight.
Heating immediately after pouring the silicone can accelerate curing
Heating immediately after pouring the silicone will cause the curing agent to volatilize, resulting in incomplete curing. It is necessary to heat after the initial curing of the liquid silicone.
Natural exhaust after stirring is sufficient
For condensation-type mold silicone, vacuum exhaust for bubbles needs to be carried out. Otherwise, bubbles will remain in the details of the mother mold, and it is prone to tearing during mold flipping.
A little more curing agent leads to faster and better curing
Excessive curing agent will make the mold brittle and reduce its tensile strength. The number of mold flips will actually decrease. It is necessary to accurately proportion by 100:2.
Compatible with the mother mold can directly pour the silicone
It is still necessary to confirm the surface cleanliness, release agent, proportion, bubble removal, pouring and curing conditions.
25℃ performance is the same, so equal quantities can be substituted
The hardness, viscosity, tensile strength and elongation of the 7 models vary significantly. When substituting, it is necessary to re-verify the bubble removal, release and mold flipping performance.
The product mold silicone 800/900 series can be used for all mold production
This series is suitable for condensation-type gypsum, cement, resin molds, high transparency jewelry, high-temperature baking molds or systems with special flame retardant requirements. It may be necessary to choose add-on mold silicone for such cases.
Curing hardness reaching the standard indicates more mold flips
The number of mold flips also depends on the tensile strength, resistance to resin heat release, release method and repeated use conditions. Actual mold flipping verification is required.
Recommendation for selection steps
Confirm the application direction: gypsum, cement, POLY-RESIN, PU, AB water, ABS molds or oil clay, toys, gifts, sculpture replication.
Confirm the type of mother mold, surface treatment and compatibility with the release agent.
Confirm the mold frame material and curing agent type and condition.
Confirm the target hardness, tensile strength, elongation and stretch.
Confirm the viscosity of the rubber and vacuum bubble removal equipment conditions.
Confirm the A/B weight ratio, stirring, pouring and curing conditions.
Select the hardness model of the product mold silicone 800/900 series based on the structure of the mother mold and resin type.
Set up different models, bubble removal and curing conditions gradients for small tests.
Test bubbles, hardness, tensile strength, elongation, shrinkage rate and contraction rate.
Carry out actual resin mold flipping, release, mold flipping times and mold lifespan verification.
Evaluate the consistency of curing among batches and the fluctuation of mold flipping performance.
Confirm that the curing agent is moisture-proof, does not heat immediately after pouring, and the vacuum bubble removal is in place.